Raw Material Guides

Wall Putty Raw Material List: White Cement, Calcite, RDP and IS 17545

What goes into cement-based and acrylic wall putty, what each raw material does, and the Indian Standard

Team Lithionyx ChemicalsSourcing & Technical Desk11 min read
Painter spreading white wall putty on an interior wall with a steel trowel

Cement-based wall putty is a fine white powder made mostly of mineral filler (calcite, often with dolomite) bound by white cement, with small amounts of redispersible polymer powder (RDP) for adhesion and flexibility and a cellulose ether such as MHEC to hold water. Acrylic wall putty is a ready-mixed paste of fine fillers bound by an acrylic or styrene-acrylic emulsion. In India, white cement-based putty is covered by IS 17545:2021, "White cement based polymeric putty".

Putty is spread in thin coats over plaster to fill fine cracks and give a smooth base for paint. Technical literature on skim coats puts a single layer at about 0.5–2 mm. This guide lists the raw materials, gives indicative ranges from published studies and supplier literature, and explains water retention, open time and the standard.

How to use this guide. The ranges and the example batch are typical starting points taken from published formulation literature and Indian Standards. They are not a tested recipe. Run small trial batches, test the finished product (ideally in an NABL-accredited lab) and follow each raw material's Safety Data Sheet. Lithionyx Chemicals supplies raw materials; we do not manufacture or test finished products.

Wall putty raw material list (white cement-based powder)

Raw materialJobIndicative % of the dry mix
White cement (white Portland cement, IS 8042)Binder: sets hard, gives strength and whitenessAbout 20–35%
Calcite powder (10 micron) or ground calcium carbonateMain filler: body, smooth finish, low costBalance, often the largest single item
Dolomite powder (fine)Second filler, used with or instead of calcitePart of the filler balance
Whiting (chalk powder)Low-cost filler in economy puttiesPart of the filler balance
Talc (10 micron) or talc powderPlaty filler: smoother trowelling and sandingSmall amounts
Redispersible polymer powder (RDP)Adhesion, flexibility, less water absorption, fewer cracksAbout 1–2.5%
MHEC (methylhydroxyethyl cellulose)Water retention, open time, workability, sag resistanceAbout 0.2–0.5%
Calcium stearate (optional)Water repellency for damp or humid wallsSmall dose, per supplier TDS
Gloss powder or whitening gloss powder (optional)Trade additives for sheen and smoothness in gloss puttiesPer supplier; trial first

No published BIS formula exists for wall putty; the standard tests the finished product, not the recipe. The ranges above are indicative and come from a published skim coat study, supplier technical data and the composition notes summarised in the standards section below.

What each raw material does

1. White cement: the binder

White cement reacts with the mixing water and sets, locking the fillers into a hard, white layer. It is what makes the putty water-resistant once cured. Too little cement and the surface stays soft and powdery; too much raises cost and can make the coat harder to sand. Use white Portland cement to IS 8042; grey cement spoils the whiteness.

2. Fillers: calcite, dolomite, talc

Fillers make up most of the bag. Skim coats use fine calcium carbonate rather than sand, which is why putty gives a glass-smooth finish. Calcite and dolomite give body and whiteness; a small amount of talc, whose particles are flat plates, helps the trowel glide and the dried coat sand evenly. Ask for particle size (for example, 10 micron), whiteness and moisture on the COA: coarse or damp filler shows up as scratches and lumps.

3. Redispersible polymer powder (RDP)

Cement on its own is brittle and can crack under the movement and temperature changes of a wall. RDP is a spray-dried polymer (most often a vinyl acetate-ethylene copolymer) that turns back into tiny polymer particles when the putty is mixed with water. As the putty dries, these form flexible bridges between the filler and cement grains, raising adhesion and flexibility and cutting water absorption. A 2020 study on white cement skim coats found adhesion and flexural strength rose with RDP dosage up to 2.5%, while compressive strength and water absorption were best at about 1–1.5%.

4. Cellulose ether (MHEC)

MHEC dissolves in the mixing water and holds it against evaporation and against the suction of a dry wall. That lets the cement hydrate properly, keeps the paste workable for longer and stops it sliding off the trowel. Usual dosage is about 0.2–0.5% of the dry mix; grades differ widely in viscosity, so name the viscosity and test method when you order. Cellulose ethers can slow cement setting, so do not overdose.

Water retention, open time and pot life

  • Water retention is how well the wet putty keeps its water on a porous wall. Poor water retention means the wall sucks the water out, the cement cannot set fully and the coat cracks or powders. IS 17545 includes a water retentivity test.
  • Open time is how long a spread coat stays workable before it skins over. MHEC and RDP both extend it.
  • Pot life is how long mixed putty stays usable in the tub. Once the cement starts to set, adding more water weakens it. Mix only what can be used within the time stated on your bag, and never re-mix stiffened putty with extra water.

Indicative 100 kg white cement putty dry mix

Indicative 100 kg white cement wall putty dry mix: calcite, white cement, dolomite, talc, redispersible polymer powder and MHEC

Indicative only, assembled from published ranges. Trial it and test against IS 17545 before you sell.

Dry-blend the powders in a ribbon or plough mixer until uniform, then pack in moisture-proof bags. On site, the powder is added to clean water and mixed to a smooth paste; the 2020 study mixed 35 parts of water per 100 parts of powder. Find the water ratio for your own mix by trial and print it on the bag.

Acrylic wall putty (paste) raw materials

Acrylic putty is sold ready to use in tubs. It is a water-based paste, closer to a very thick, high-filler paint than to a cement product. It dries rather than sets, so it does not need cement or curing.

Raw materialJobIndicative level
Styrene-acrylic emulsion or styrene-acrylic binderBinder: adhesion and film strengthDecides adhesion and cost; set by trials
Calcite (10 micron) and talcFillers: body, smoothness, sandingMost of the paste
HEC (hydroxyethyl cellulose)Thickener and water retention; stops settlingSmall amounts
Sodium polyacrylate dispersantWets and disperses the calcite, lowers paste viscositySmall amounts
DefoamerStops air bubbles and pinholesSmall amounts
In-can preservativeStops the paste rotting or smelling in the tubPer supplier TDS
WaterCarrierBalance

We did not find a reliable published starting formula for acrylic paste putty, so we give no percentages here. Work from your binder supplier's guidance and test adhesion, sanding, cracking on thick coats and shelf life.

Cement-based or acrylic putty?

White cement-based powderAcrylic paste
FormDry powder, mixed with water on siteReady-mixed paste in a tub
BinderWhite cement plus RDPAcrylic or styrene-acrylic emulsion
How it hardensCement sets (chemical reaction)Water evaporates
Typical useInterior and exterior plastered wallsInterior walls; exterior only with a binder rated for it
Main risksShort pot life, cracking if it dries too fastSpoilage in the tub, shrinkage in thick coats

IS 17545 and testing

The BIS standard IS 17545:2021 White cement based polymeric putty covers putty used as a finished skim coat on internal or external plastered surfaces. Certification guidance lists the characteristics it tests: consistency, water retentivity, setting time, polymer content, cement content, degree of whiteness, tensile adhesion strength and a lead restriction.

A public draft East African standard adapted from IS 17545 says white cement shall be the key ingredient and asks for at least 1.5% pure polymer by mass, at least 18% cement content and at least 85% whiteness. We have not read the Indian text, so treat these as indicative and check the limits in IS 17545 itself before you test. Note that RDP as supplied is not 100% polymer, so allow for this when you plan to meet a polymer minimum.

Whether BIS certification is compulsory for wall putty should be checked with BIS at the time you launch. We did not find a Quality Control Order for it. Tile adhesive is a separate product with its own standard, IS 15477.

Common problems

  • Hairline cracks: coat too thick, wall too dry or hot, too little RDP or cellulose ether. Apply thin coats and dampen very absorbent walls.
  • Powdery surface: too much water in the mix, too little cement or polymer, or the coat dried before the cement could set.
  • Peeling or poor adhesion: dusty, oily or damp substrate, or low RDP.
  • Mould, blisters or cracks on damp walls: constant moisture. Fix the leak first; hydrophobic additives help only on walls that dry out.
  • Lumps in the mixed paste: powder dumped into water too fast, or cellulose ether that did not wet out. Add powder to water slowly while mixing and let it stand a few minutes before re-stirring.
  • Pinholes and bubbles (acrylic paste): trapped air. Check the defoamer and avoid over-fast mixing.

Safety and handling

  • Wet cement is strongly alkaline and can burn skin and eyes. Wear gloves and goggles when mixing and applying putty.
  • Cement, calcite, dolomite and talc dust irritate the eyes and lungs. Use dust extraction and masks at the mixer and the packing point.
  • Calcium stearate and other fine organic powders can form explosive dust clouds; avoid dust build-up.
  • Store cement-based putty and RDP dry and cool; damp bags set into lumps. Follow each raw material's Safety Data Sheet, and see COA vs SDS for what those documents should contain.

Frequently asked questions

What raw materials are used to make wall putty?

White cement, fine calcite or dolomite powder, a little talc, redispersible polymer powder (RDP) and a cellulose ether such as MHEC. Acrylic putty uses an acrylic emulsion binder, calcite, talc, HEC, dispersant, defoamer, preservative and water.

What is wall putty made of: cement or chalk?

Both. Most of a bag is fine mineral filler such as calcite (a form of calcium carbonate, like chalk), held together by white cement and a polymer.

How much RDP is used in wall putty?

Typically about 1–2.5% of the dry mix. A published skim coat study found the best balance of strength and low water absorption at about 1–1.5%, with adhesion still rising up to 2.5%.

Which BIS standard applies to wall putty?

IS 17545:2021, White cement based polymeric putty. IS 15477 is for tile adhesives, not putty.

Why does wall putty crack?

Usually because the coat is too thick, the wall pulled the water out too fast, or the mix has too little polymer or cellulose ether. Apply thin coats and check the water ratio.

हिंदी में सार

वॉल पुट्टी बनाने का रॉ मटेरियल / फार्मूला: सफ़ेद सीमेंट, बारीक कैल्साइट या डोलोमाइट पाउडर, थोड़ा टैल्क, RDP (रीडिस्पर्सिबल पॉलिमर पाउडर) और MHEC सेल्युलोज़ ईथर। एक्रेलिक पुट्टी में सीमेंट की जगह एक्रेलिक इमल्शन बाइंडर लगता है। ऊपर दी गई मात्राएँ केवल अनुमान हैं; बेचने से पहले ट्रायल बैच बनाकर IS 17545 के अनुसार टेस्ट कराएँ।

Buy the raw materials from one supplier

Lithionyx Chemicals supplies calcite, talc, whiting, redispersible polymer powder, MHEC, HEC, calcium stearate and styrene-acrylic binders to manufacturers across India, with export on order. Every batch ships with the manufacturer's Certificate of Analysis and Safety Data Sheet, and we confirm grade, packing and dispatch before we quote. Send us your full raw material list with monthly quantities using the Request a Quote button, or write to hello@lithionyx.com, and we will quote the whole list in one go.

Sources

  • BIS, IS 17545:2021 White cement based polymeric putty (BIS "Know your standards" listing and the BIS construction materials category list).
  • Certification guidance on IS 17545 listing its test characteristics (Elitas).
  • Tanzania Bureau of Standards, draft standard BCDC 9 (3570) DTZS, white cement based polymeric putty, adapted from IS 17545, as quoted in search indexes (not read in full).
  • Wickramanayaka S., "Improving properties of cement based skim coat through controlling water absorption using a vinyl acetate-ethylene copolymer", MSc thesis, University of Moratuwa, 2020.
  • Wacker Chemie, "Construction: skim coat" technical article (calcium carbonate filler, role of polymer, 0.5–2 mm layers).
  • BIS, IS 8042 White Portland cement; IS 15477 Adhesives for use with ceramic, mosaic and stone tiles.
  • Manufacturer technical data for RDP, MHEC and calcium stearate.
  • Construction Chemicals
  • Paints & Coatings
  • Raw Material Guide
Written by

Team Lithionyx Chemicals

Sourcing & Technical Desk

Our sourcing and technical desk in Vadodara works with manufacturers across India every day on grades, documents, packaging and dispatch. These notes share what we learn along the way.

Keep reading

All articles

10 min read

SLES 70% vs SLES 28%: Differences, Dilution and Which to Buy

SLES 70% and SLES 28% are the same surfactant with different amounts of water. This guide explains the difference, how to dilute the 70% paste without a gel, how to convert a formula between grades, how to compare offers per kg of active and what to check on the COA.

Team Lithionyx Chemicals
Bonded by Trust. Driven by Courage.

Tell us what you need. We’ll get back to you.

Product, grade, quantity and delivery location are all we need to start. Our sourcing desk replies within one business day, with the manufacturer’s COA and SDS for every batch.